چكيده لاتين :
Molybdenite flotation in the Sarcheshmeh Copper Complex was studied as a function of pulp potential, controlled using two types of sodium sulfide, a mineral origin and a chemical nature. Air and either plant or laboratory nitrogen were used as flotation careers. Potential readings took place in rougher cells, as it was proved to be vital in the molybdenite circuit. Results showed that, at reducing potentials between -525 and -575 mv, the highest molybdenum recovery of 93% and the lowest copper recovery of 4-15% can be achieved. These potentials did not change considerably by adding extra amounts of sodium sulfide. At more oxidizing potentials, i.e. more than -450 mv, copper recovery increases while the recovery of Molybdenite drops.